PRECIPITATION-HARDENING STAINLESS STEEL

15-5PH Stainless SteelUNS S15500 · XM-12

Kongfang Metal supplies 15-5PH stainless steel plate, sheet, strip, bars, forgings and machined components, with stock, warehousing and processing services. This precipitation-hardening grade is used for parts requiring high strength, toughness and corrosion resistance. Send your dimensions, quantity and required delivery condition.

Plate, sheet & stripBar & forgingsH900 to H1150MTest direction matters
15-5PH stainless steel bars and machined components
Confirm the purchase identity15-5PH / UNS S15500 plus the product-specific standard
Define the conditionCondition A is the solution-treated starting condition before final aging
Control critical sectionsMelt route, specimen location and test direction can affect acceptance
Quick selection guide

Start With the Requirement, Then Confirm the Route

Select the aging condition for the required balance of strength, toughness and corrosion resistance. Use the product standard, section size, service environment and required tests to complete the order specification.

If the requirement isStart withConfirm before ordering
High strength after a single aging treatment15-5PH in an age-hardened conditionGoverning standard, starting condition, aging condition and minimum properties
Better transverse-property consistency than a conventional 17-4PH route in a critical section15-5PH may be appropriateProduct size, melt/remelt route, test location and direction, and the specified result
Maximum room-temperature strengthH900 is commonly considered firstToughness, stress-corrosion exposure, fatigue, section size and whether the standard permits the condition
Greater toughness and ductilityConsider H1025, H1100 or H1150Minimum strength, impact requirement, section and service environment
Persistent seawater, chloride cleaner or crevice exposureReassess the material choiceTemperature, chloride concentration, pH, wet time, stress and cleaning regime
A welded high-strength assemblyReview the complete procedureStarting condition, filler, restraint, heat input, interpass control and post-weld heat treatment
First enquiry: send the product form, approximate dimensions, quantity, destination and any condition shown on the drawing. If the condition is undecided, include the application and operating environment.
Available forms and supply options

15-5PH Stock and Processing

We supply 15-5PH material and components made to your drawing. Send the material specification and delivery condition, plus any melt-route or test-direction requirements.

Supply summary

Prepare your quotation request with the material, processing, document and delivery requirements below.

Applicable specificationWe confirm the flat-product, bar, forging or customer specification used for the quotation.
Condition and processingCondition A (the solution-treated starting condition) or the required aged condition, cutting, machining allowance and heat-treatment responsibility are agreed for the order.
Documents and inspectionInclude your MTC, heat/lot traceability, PMI, mechanical or impact testing, NDT and third-party inspection requirements in the order.
Quote basisYour quotation covers the material dimensions, processing, documents and delivery plan.
Grade identity and product standards

Specify 15-5PH / UNS S15500 With the Product Standard

The alloy is also identified as XM-12 in ASTM/ASME designation tables. The product standard still governs the ordered material. SUS 631 refers to 17-7PH and should not be used as a 15-5PH purchase identity.

Product routeCommon specification to reviewWhat the scope tells the buyer
Plate, sheet and stripASTM A693Precipitation-hardening stainless flat products whose properties are developed by low-temperature aging
Hot-rolled or cold-finished bars and shapesASTM A564/A564MThe ordered condition and mechanical requirements still need to be stated
General-purpose forgingsASTM A705/A705MThe order must state the grade, condition, properties and supplementary inspection
Premium aerospace bars, wire, forgings, rings and extrusionsSAE AMS5659Consumable-electrode-remelted 15-5PH long-product and forging routes
Premium aerospace sheet, strip and plateSAE AMS5862Consumable-electrode-remelted 15-5PH flat products; condition-specific slash specifications may apply
If another national designation appears on the drawing: resolve it against the required chemistry, product form and properties before accepting a substitution.
Composition and melt route

Chemistry Confirms the Alloy Family—Not the Final Condition

UNS S15500 composition

Mass-percent ranges suitable for grade identification.

ElementUNS S15500
Carbon (C)≤ 0.07
Silicon (Si)≤ 1.00
Manganese (Mn)≤ 1.00
Phosphorus (P)≤ 0.040
Sulfur (S)≤ 0.030
Chromium (Cr)14.0–15.5
Nickel (Ni)3.50–5.50
Copper (Cu)2.5–4.5
Niobium + tantalum0.15–0.45
Iron (Fe)Balance

The governing product standard and the supplied heat's material certificate control acceptance.

Why melt route and test direction matter

15-5PH was developed from the 17-4PH family with the aim of reducing delta-ferrite-related variation and improving short-transverse properties. Properties can still vary through a large bar or forging.

Critical-Section Requirements

  • required melt or remelt route;
  • test direction and specimen location;
  • final condition and minimum properties;
  • separate coupons, prolongations or product testing.

If transverse properties are critical, include the test direction, sampling location and minimum acceptable result.

Heat-treatment conditions

Condition A Is the Starting Point; Aging Sets the Balance

Lower aging temperatures generally emphasize strength. Higher aging temperatures or double overaging trade some strength for greater ductility and impact resistance.

ConditionHistorical reference cycleSelection meaning
Condition A1900°F ± 25°F (about 1038°C ± 14°C) for 0.5 h, then oil or air coolStarting condition for machining and subsequent aging
H900900°F (482°C) for 1 h, air coolHighest strength and hardness among the listed standard conditions; verify toughness and environment
H925925°F (496°C) for 4 h, air coolSlightly lower strength than H900 with a modest shift toward ductility and toughness
H10251025°F (552°C) for 4 h, air coolCommon intermediate balance; confirm the drawing's required properties
H10751075°F (579°C) for 4 h, air coolFurther reduction in strength with increasing ductility and impact response
H11001100°F (593°C) for 4 h, air coolUsed where the requirement moves away from maximum strength
H11501150°F (621°C) for 4 h, air coolHigher ductility and toughness than lower-temperature aging conditions, with lower strength
H1150M1400°F (760°C) for 2 h, air cool; then 1150°F (621°C) for 4 h, air coolDouble-overaged route when toughness and stress-corrosion considerations outweigh maximum strength

Source: NASA SP-5089, Table XII, p. 57. Use the cycle required by the current product specification and qualified procedure.

Historical material data

Typical Mechanical-Property Trend by Condition

These selected historical values are for longitudinal specimens from an intermediate location in bar stock. Use them to compare the direction of change—not as minimum acceptance values or design allowables for another product form or heat.

ConditionUTS, ksi (approx. MPa)0.2% yield, ksi (approx. MPa)ElongationHardnessCharpy V-notch, ft·lbf (approx. J)
H900200 (1380)185 (1275)14%44 HRC20 (27)
H1025170 (1170)165 (1140)15%38 HRC35 (47)
H1100150 (1035)135 (930)17%34 HRC45 (61)
H1150145 (1000)125 (860)19%33 HRC50 (68)
H1150M125 (860)85 (585)22%27 HRC100 (136)

Source: NASA SP-5089, Table XIII, p. 58. The source table does not state the Charpy test temperature or specimen size. Specify impact-test acceptance requirements separately.

15-5PH / UNS S15500

Transverse-Property Requirements

Consider 15-5PH when transverse-property consistency is a key requirement. Compare the required strength and toughness at the specified aging condition, section size and test direction.

17-4PH / UNS S17400

Compare Stock Sizes, Processing and Delivery

If both grades meet the required properties, compare stock sizes, processing and delivery for the actual component. See our 17-4PH grade guide for its conditions and product options.

Corrosion resistance and service limits

Assess Chlorides, Stress and the Aging Condition Together

15-5PH offers useful corrosion resistance for a high-strength martensitic PH alloy, but persistent seawater, acidified chloride, warm chloride cleaners, crevices or sustained tensile stress require a separate material assessment.

Review the full environment

Service exposure is more than the alloy name

Check temperature, chemistry, concentration, wet/dry cycle, stress, crevices, deposits, drainage, cleaning practice and surface condition.

TemperatureChloridesStressSurface condition
Do not use a condition name alone

High strength can change the corrosion boundary

High-strength conditions can be more sensitive to stress-corrosion cracking in aggressive environments than lower-strength overaged conditions.

SeawaterWarm cleanersCrevicesSustained stress
Application boundary

Connect the material to a measurable requirement

Common applications include aerospace fittings, shafts, valve components, fasteners and high-load parts. Key selection checks are listed below.

  • Critical structural part: standard, remelt route, test direction, condition, fatigue-critical surface and traceability.
  • Shaft or drive component: load, fatigue, diameter, straightness, condition and post-aging machining.
  • Valve or actuator part: pressure boundary, medium, chloride exposure, contact stress, galling pair and inspection code.
  • Fastener or threaded part: thread sequence, final condition, proof/load requirement and hydrogen or stress-corrosion controls.

ASTM A693 and A564 describe uses up to 600°F (315°C) within their scopes. Creep, oxidation, relaxation, coatings and application-specific design rules require separate checks.

Machining, forming and welding

Plan Fabrication Around the Final Condition

Machine most features in Condition A when the manufacturing route allows it, then age to the specified final condition. Protect traceability and agree which dimensions are inspected before and after heat treatment.

01

Machining

Leave enough allowance for final grinding or distortion correction. When bar or plate is divided, preserve heat and lot identity through the cut pieces.

02

Forming

Confirm bend radius, rolling direction, thickness and final heat treatment on the actual product. Qualify the forming rule for the product form and section.

03

Welding

Starting condition, restraint, filler, heat input, interpass temperature and post-weld heat treatment affect cracking risk and final properties.

Welding procedure: define the controls in a qualified welding procedure specification (WPS). Use the WPS to define the required joint strength and post-weld heat-treatment sequence.
Documentation and inspection

Connect the Certificate, Condition and Finished Lot

01

Material identity

The material test certificate (MTC) should identify the grade, heat or lot, governing specification, condition and chemistry.

02

Condition and properties

Heat-treatment records, hardness testing and the required mechanical or impact tests establish the delivered condition and agreed properties.

03

Traceability

Preserve heat or lot traceability when stock is cut. If a premium remelt route is required, state it in the order and verify it on the certificate.

PMI boundary: positive material identification can help verify alloying elements, but it does not establish the heat-treatment condition or replace the specified mechanical tests.
Request a 15-5PH quote

Start With What You Know

Send the form, dimensions, quantity and any condition shown on the drawing. If you are still selecting the condition, share the application and operating environment so we can help prepare the material and processing quotation.

For a formal RFQ, include as applicable

  • 15-5PH / UNS S15500 and governing specification with revision
  • product form, dimensions, tolerances and quantity
  • melt/remelt route when required
  • delivery and final aging condition
  • mechanical, hardness or impact requirements, including test direction and temperature
  • MTC, traceability, PMI, NDT or other inspection
  • processing, packaging, destination and required delivery date
RFQ example: 15-5PH / UNS S15500 round bar for machined actuator shafts; 65 mm diameter × 3 m, 2 metric tons. Drawing calls for H1025 and longitudinal tensile certification. Please confirm the applicable standard, available starting stock size, cutting allowance, MTC/traceability, lead time and delivery to Houston.
Frequently asked questions

15-5PH Purchasing Questions

Is 15-5PH the same as 17-4PH?

No. They are related martensitic precipitation-hardening stainless steels with similar aging treatments, but their UNS designations and chemistry differ. A substitution requires approval against the product specification, section, condition and required properties.

What is the correct designation for 15-5PH?

Use 15-5PH with UNS S15500 and the product-specific governing specification. XM-12 is another recognized designation. Resolve other cross-references before ordering.

Which condition is strongest?

H900 usually provides the highest strength and hardness among the listed aging conditions. Check toughness, stress-corrosion exposure, fatigue, section and the governing specification before selecting it.

What is the difference between H1025 and H1150?

H1025 generally retains more strength. H1150 generally offers more ductility and impact toughness at lower strength. Use the actual required properties and test methods, not the condition name alone.

Is 15-5PH suitable for seawater?

A seawater or aggressive-chloride application needs a separate material assessment covering chloride concentration, temperature, crevices, stress, exposure duration and aging condition.

Can 15-5PH be welded?

Yes, but it requires a qualified procedure covering starting condition, restraint, filler, heat input, interpass control and post-weld heat treatment.

Is 15-5PH magnetic?

Yes. In its normal martensitic conditions, 15-5PH is ferromagnetic.

What should I include in a 15-5PH enquiry?

Send the product form, dimensions and quantity, with any required condition, standard or drawing. Add your processing, inspection, documentation and delivery requirements so we can include them in the quotation.